This temporature. The scientific answer is 80% of the head distortion temporary (HDT). Any cooler is a was a waste of time.
FIXTURE ALLOWING A TEN-MINUTE Air COOL While Clamped in the Proper Geometry. Produblem Solved.
liquid. But if they become solid too quickly, you now have a part with a laarge amount of internaly and it will definitly warp.
PROBLEM HERE WASN’T Heat Transfer From The Steel to the Plastic; It was the factic is a really poor compasser of heat so it takes a long time to companys 80% HDT to remian state.
We did’T do any queenching. At the end of this project, they we molding parts at 29 Seconds/Cycle and Still Sealing they at the Machine Rate with The Two-Minute Cycle!
Tricks when the cuscomer pulls the job
Tricks Molded Case Parts and Enjoy the Profits. If you must give your custer proces conditions do the footowing:
MOLD-MOUNTED WATER Manifolds and Balance them. Take the thatm off and ship the mold out of sater-line diagrams.
It’s your choice.
Bill Tobin is a consultant who teaches seminars and helps clients improve their productivity. He can be contacted at www.wjtassociates or via e-mail at.
Read the Previous Articles in this molded cases series:
"Molding Tricks for Higher Profits: The Expert Syndrome" "" "
"Molding Tricks for Higher Profits, Part 2: The Philosophy" "" "
"Molding Tricks for Higher Profits, Part 3: The Mold"
"Molding Tricks for Higher Profits, Part 4: Filling The Mold"